Overview
Abrasion resistance is how well a coating stands up to being worn away. The Taber test puts a number on it by wearing a sample under controlled conditions and weighing the loss.
What the test measures
The test measures the mass of coating removed by a fixed amount of rubbing wear. The result is given in milligrams lost.
How the test is carried out
The Taber abraser is described in several standards, including ASTM D4060, ISO 7784-2 and EN ISO 5470-1. They share one principle.
- A coated panel is cured, weighed and fixed to a turntable.
- Two abrasive wheels are lowered onto it under a set load.
- The turntable rotates for a set number of cycles. The wheels rub a ring into the film.
- The panel is cleaned and weighed again. The difference is the result.
Three settings decide how severe the test is.
| Setting | Common choice |
|---|---|
| Wheel | CS-10 or CS-17. CS-17 is the harsher of the two. |
| Load | 1000 g on each wheel. |
| Cycles | 1000. |
How to read the result
Lower is better. A coating that loses 40 mg has worn less than one that loses 120 mg in the same test.
A figure is only complete with its conditions, for example "40 mg loss, CS-17 wheels, 1000 g, 1000 cycles". Without them it cannot be compared with anything.
What it means in use
Abrasion is the everyday wear a floor sees: foot traffic, trolley and forklift wheels, and grit carried in on shoes and tyres. A lower loss figure points to a film that keeps its thickness, and its appearance, for longer under that wear.
What the result does not tell you
Results from different wheels, loads or cycle counts cannot be compared. Check the conditions before comparing two products.
The test weighs what is lost. A dense, heavily filled coating can lose more milligrams than a light one while losing no more thickness.
The Taber test is steady rubbing wear. It does not reproduce impact, tyres turning on the spot, or sharp grit being dragged under a pallet. See Impact Resistance and Scratch Resistance for those.
Screed standards use different wear tests and report classes such as AR. An AR class cannot be converted to a Taber figure.
On our product pages
Where a product has been tested, its page shows the result, the method and, where the method has one, the rating. Results published on this site come from internal testing to the stated method. They are given for technical reference and comparison.
If a figure you need is not shown, ask our technical team.



Share:
Slip Resistance (Pendulum Test)
Adhesion (Cross-Cut)